Buyer decision guide · 2026-11-25

Does an ASTM D395 compression-set value prove a PU caster will recover after a parked dwell?

No. A compression-set percentage is a material-specimen result under a defined test protocol, not a complete-wheel parked-load rating. Method, strain or force, temperature, duration and recovery interval all matter; static compression-set evidence also does not replace dynamic rolling-heat evidence.

The buyer decision

The existing distinction between a short structural overload proof and a long stationary dwell remains important, but a buyer may also receive a supplier's “low compression set” claim or an ASTM D395 report. That report is useful only when its test conditions are known and relevant. It cannot, by itself, tell you how many hours a finished wheel can remain loaded without a flat spot, how deep a flat will be, or whether the wheel will recover after unloading.

What ASTM D395 actually measures

ASTM D395-18(2025), §§1.1–1.3 and 4.1, defines three methods: A under constant force, B under constant deflection, and C under constant deflection considering material hardness. Its significance-and-use section says compression set can arise under maintained deflection, constant force or repeated deformation/recovery. However, it says dynamic effects are more closely simulated by compression-flexing or hysteresis tests and that compression-set methods are mainly applicable to static-stress service.

Therefore, “tested to ASTM D395” is incomplete as a comparison. The buyer needs the method, specimen dimensions and shape, applied force or deflection, test temperature, dwell duration, recovery interval and measured result. ASTM does not prescribe a universal pass percentage for industrial caster wheels, nor does it turn a coupon result into a 12-hour, 24-hour or multi-day wheel rating.

Why same Shore A hardness can still produce different results

Anderson Development's A Practical Look at Compression Set: Effect of Temperature and % Deflection tested cast 1/2-inch polyurethane buttons using ASTM D395 Method B. Samples were post-cured and conditioned at 23°C / 50% relative humidity for at least one month; they were then held for 22 hours at 25, 50, 70 or 85°C and allowed 2 hours of ambient recovery. The study varied deflection from 3% to 25% and compared PTMEG- and ester-based soft segments, MBOCA and DMTDA curatives, and formulation stoichiometry.

Anderson Development specimenMatched test conditionsCompression setWhat the comparison shows
85A LFTDI/PTMEG/MBOCA, stoichiometry 0.95Method B; 25% deflection; 22 h; 25°C7%Same formulation, higher test temperature: 25°C to 70°C changes the reported value.
Same 85A PTMEG/MBOCA specimen familyMethod B; 25% deflection; 22 h; 70°C18%
85A LFTDI/ester/MBOCA, stoichiometry 0.95Method B; 25% deflection; 22 h; 70°C25%Same nominal hardness and matched protocol, different soft-segment chemistry: the reported value differs from the PTMEG result.

These are the paper's material-specimen results, not finished-wheel tests. They show why a buyer cannot infer compression-set equivalence from “85A PU” alone. They do not prove that every ester PU has a higher set than every polyether PU, and they do not predict a particular caster's flat depth.

Compression set is not the same as creep or dynamic wheel behaviour

Boedeker Plastics' Polyurethane — Technical Guide explicitly separates compression set (deformation remaining after stress is removed), creep (deformation increasing over time under constant stress) and stress relaxation (stress decreasing under constant deformation). It warns that short compression-set tests suggest rather than predict long-term service behaviour. It also states that creep depends on initial strain and temperature, and that dynamic loading can increase creep through internal heat generation.

This matters because a wheel parked for a long period is a sustained-load problem, while a wheel repeatedly rolling under high load has cyclic deformation and hysteresis heat. A static coupon result can help screen a compound for parked-load behaviour; it cannot qualify the complete wheel for continuous rolling. Conversely, a dynamic load rating does not automatically establish a wheel's long stationary recovery.

Why an unqualified compression-set range cannot rank wheel suppliers

Mearthane Products Corporation's current “Polyurethane Wheels” page publishes a 5–40% compression-set range for Durethane S and 17–20% for Durethane XL, and describes low compression set as relevant to keeping a parked wheel round. However, the public page does not pair those ranges with a specific ASTM method, specimen shape, deflection/force, temperature, dwell or recovery interval. The ranges therefore cannot be ranked against Anderson's specific test results or another supplier's number. A lower percentage is meaningful for comparison only after the underlying test conditions and compound identity are aligned.

What to request before approving a parked-load replacement

  1. Identify the exact compound: manufacturer, formulation or grade designation, nominal hardness and whether the tread is cast, molded or otherwise constructed.
  2. Obtain the complete coupon protocol: ASTM D395 method (A/B/C), specimen dimensions and shape, conditioning, force or deflection, temperature, dwell duration, recovery interval and measured result.
  3. State the actual wheel duty: maximum reaction per wheel, wheel diameter and tread width/thickness, core construction, floor, ambient and wheel temperature, and uninterrupted parked duration.
  4. Request wheel-level evidence: test the exact wheel construction at the representative load and temperature; record loaded deformation, dwell, unloaded recovery time, residual tread/diameter/runout and whether restart produces unacceptable vibration or push force.
  5. Keep rolling qualification separate: for continuous or repeated movement, request representative rolling-duty evidence addressing speed, load, cycle, heat build-up and acceptance criteria.

Practical rejection rule: if a supplier provides only Shore hardness, “low compression set”, or an ASTM D395 percentage without its method and conditions, record parked-load recovery as not demonstrated. This is not proof that the wheel will fail; it means the evidence does not qualify the buyer's dwell condition.

Evidence boundary

The Anderson values apply only to its stated cast specimens and protocol; they are not wheel-diameter losses. Boedeker's examples apply to its Die-Thane compounds and are not a general caster rating. Mearthane's published ranges lack the conditions needed for direct numerical comparison. No cited source establishes a universal compression-set threshold for caster wheels, a conversion from coupon percentage to flat depth, or a universal parked duration. No wheel-level dwell/recovery test for this supplier's products is claimed.

Sources: ASTM International, ASTM D395-18(2025), Standard Test Methods for Rubber Property—Compression Set, active edition D0395-18R25 (last updated 2025-02-21), §§1.1–1.3 and 4.1, https://store.astm.org/d0395-18r25.html. Anderson Development Company, Stephen Seneker, Caleigh Elliott and Jordan Duckett, A Practical Look at Compression Set: Effect of Temperature and % Deflection, consulted PDF undated, printed pp.1–14, especially pp.2–3 and pp.12–14 appendices, https://www.andersondevelopment.com/pdf/PU%20Technical%20Papers-added%2003162021/Study%20of%20Effect%20on%20Compression%20Set.pdf. Boedeker Plastics, Polyurethane — Technical Guide, PDF version stamp 2020-12-18, “Engineering Property — Compression Set, Creep & Stress Relaxation” and “Creep”, PDF pp.11–12, https://www.boedeker.com/Portals/0/Documents/Boedeker%20Plastics%20Polyurethane%20-%20Technical%20Guide.pdf?ver=2020-12-18-173355-917. Mearthane Products Corporation, “Polyurethane Wheels”, current manufacturer page accessed 2026-11-25, “Flat-spotting” and “The specs that matter”, https://mpcurethane.com/products/polyurethane-wheels/.