1. The buyer problem: grade name versus the real corrosion site
“Stainless steel” and even “316” are not complete wet-service qualifications. Caster metalwork can include plates, forks, fasteners, axles and swivel/bearing interfaces. A washer/bolt contact, folded edge, intermittent weld, deposit or tight interface may retain a small volume of chloride-bearing liquid. The question is not only whether the exposed alloy resists pitting, but whether the actual joint can remain wet and concentrate salts.
Decision in brief: 304 is not a seawater-service default. 316 is a meaningful alloy upgrade in many chloride environments, but it remains susceptible to local pitting and crevice corrosion. If the design traps brine or deposits, first address drainage, cleaning and crevice geometry; if severe exposure remains, obtain an application-specific assessment of higher-alloy or duplex options. This is a screening path, not a universal grade recommendation.
2. Independent sources and original evidence
Source A — Australian Stainless Steel Development Association (ASSDA)
Document: “Crevices and Corrosion,” current online technical article, accessed 2026-11-25.
Location: “Why crevices can corrode”; Table 1 “Critical temperatures required to cause pitting”; “Crevice Shape,” “Environment,” “Temperature,” “Alloy Resistance” and prevention guidance.
URL: https://assda.asn.au/stainless-steel/properties-and-performance/crevices-and-corrosion
- ASSDA describes crevices under washers/bolt heads, between bolted plates, intermittent welds and gasket interfaces. Restricted oxygen renewal and stagnant moisture allow chlorides to concentrate and local chemistry to become acidic.
- Its Table 1 is based on a metal plate beneath a PTFE washer in 10% ferric chloride. It reports 304: CCT below −10°C, CPT 3°C; 316: CCT −10°C, CPT 10°C. For both grades, the listed crevice-corrosion temperature is at least 20°C below the corresponding pitting temperature.
- It says narrower/deeper crevices are worse; deposits and oxidising liquids can increase risk; higher temperature accelerates attack after the CCT is exceeded. It gives ambient-seawater examples of crevice formation at 0.9 mm gaps for 304 and 0.4 mm for 316, but these examples are not universal design clearances.
Interpretation limit: the ferric-chloride/washer results are accelerated laboratory evidence, not operating-temperature limits for a caster. The gap examples are specific to the cited seawater context, not a general minimum-gap rule.
Source B — British Stainless Steel Association (BSSA)
Document: “Selection of 316, 304 and 303 types of stainless steels for seawater applications,” current online technical article, accessed 2026-11-25.
Location: “Introduction,” “Seawater quality,” “Water flow rates,” “Water temperature” and “‘Engineered’ crevices (surface finish and post fabrication cleaning).”
- BSSA states that 316 is susceptible to localised pitting and crevice corrosion in seawater and is not corrosion-proof; 304 should not be considered suitable for seawater service.
- Evaporation can concentrate chlorides in damp splash zones. Stagnant water and slow flow promote biofouling/shielding; higher temperature increases crevice-corrosion risk.
- It identifies geometry, gaskets and mechanical fasteners as crevice sources and says surface finish, weld quality and post-fabrication cleaning can be as important as chloride concentration.
- For welded 316 structures it notes that low-carbon 316L grades such as 1.4404 or 1.4432 can avoid an additional sensitisation-related intergranular-corrosion risk; this does not remove chloride crevice risk.
Interpretation limit: this guidance concerns seawater systems and does not certify a particular caster construction or every low-chloride washdown environment.
Source C — Outokumpu Oyj
Document: Handbook of Stainless Steel, Edition 1.1 (2017).
Location: Chapter 6, printed pp. 34–36, “Pitting and crevice corrosion,” “Resistance to pitting and crevice corrosion,” Table 6:1 and Figure 6:6.
- Outokumpu says chloride-bearing media can cause pitting/crevice corrosion; under unfavourable conditions even chloride below 100 ppm can cause attack. Increasing temperature, low pH and oxidising chemicals such as chlorination increase probability.
- Its Table 6:1 lists 4301/4307 (304/304L family) at PRE 18, ASTM G48 Method E CPT 10°C and Method F CCT below 0°C; 4401/4404 (316/316L family) at PRE 24, CPT 20°C and CCT below 0°C.
- It explains that Method E uses a 24-hour acidified ferric-chloride exposure for CPT and Method F adds PTFE crevice formers for CCT. CCT values are considerably lower than CPT values.
- It explicitly warns that CPT values from different methods cannot be compared and that standard-test CPT/CCT values rank alloys but do not predict attack in a specific service environment. PRE is only a rough pitting-resistance indicator.
Interpretation limit: Outokumpu's values are test results for named grade families under the stated methods, not field-life data. The table's “below 0°C” CCT entries do not prove the grades are identical; they show that the reported test bound does not distinguish them further.
3. Cross-source differences and comparability
| Evidence dimension | ASSDA | Outokumpu | What can be concluded |
|---|---|---|---|
| Test solution / fixture | 10% ferric chloride; PTFE washer crevice | ASTM G48: acidified ferric chloride; Method F uses PTFE crevice former | Both show crevice attack can occur below open-surface pitting conditions, but their numeric temperatures must not be merged. |
| 304-family versus 316-family | 304 CCT <−10°C / CPT 3°C; 316 CCT −10°C / CPT 10°C | 4301/4307 PRE 18, CPT 10°C, CCT <0°C; 4401/4404 PRE 24, CPT 20°C, CCT <0°C | Both sources show an advantage for 316-family pitting indicators. In Outokumpu's table, the reported Method F CCT bound does not separate the families; ASSDA shows only a modest difference in its own test. |
| Real seawater context | Explains oxygen depletion, chloride concentration and geometry effects in crevices | Explains chloride, temperature, pH, oxidiser and deposit effects; says test values are not service predictions | Use the alloy data as screening evidence, then qualify the actual wet joint and operating environment. |
These are independent technical sources, not reproductions of one manufacturer's datasheet. Their laboratory protocols are not identical, so the values are not pooled or ranked across sources. The useful cross-source result is qualitative and decision-oriented: 316 improves pitting-related indicators, but crevice corrosion remains a distinct weak point, and a material-only upgrade does not remove the geometry and exposure mechanisms that create the crevice.
4. Cross-analysis: when the grade upgrade is not the first fix
- Open, freely drained surface: a grade comparison based on pitting resistance is relevant, but the exact chloride concentration, temperature, oxidiser and exposure frequency still need to match the application.
- Wet bolt/washer or joint interface: crevice chemistry can be more aggressive than the exposed surface. A 316 label is not proof that a trapped wet joint is safe.
- Salt splash followed by evaporation: the chloride concentration in the retained film can rise as water evaporates. A low average concentration measured in the bulk wash water may not describe the local deposit at the joint.
- Standing seawater or stagnant brine: BSSA explicitly cautions that 316 has limited seawater resistance. Do not approve it by grade name alone; seek geometry-specific assessment and consider drainage, cleaning and higher-alloy options together.
- Welded construction: 316L can reduce sensitisation-related intergranular risk in welded structures, but it is not a substitute for crevice-free weld geometry, cleaning or a chloride exposure assessment.
5. Procurement and RFQ decision path
- Require exact grade/UNS/EN designation and material evidence for each relevant part; “stainless steel” is not enough.
- Describe chloride source and concentration, splash/intermittent/standing/immersion exposure, maximum temperature, wet dwell, evaporation, rinse and drying frequency, and any oxidising cleaner.
- Request a drawing or close-up of fasteners, washers, folds, weld roots, bearing shields, swivel interfaces and polymer-to-metal contacts where liquid or deposits can remain.
- Ask how the assembly drains and is cleaned; specify surface finish, weld completion, post-weld cleaning and passivation where applicable.
- If a CPT/CCT report is offered, require method/standard, solution chemistry, crevice former, surface preparation, test temperature steps, sample identity and acceptance criterion. Do not compare CPT from different methods or treat a laboratory rank as a service guarantee.
- For persistent seawater, concentrated brine, heated chloride or inaccessible wet crevices, require an application-specific corrosion assessment rather than automatic approval of 316 or automatic substitution to duplex.
6. Buyer capability gained
The buyer can now distinguish an alloy upgrade from a complete corrosion qualification. They can reject the assumption that 316 means seawater-proof, recognise when a pitting rating says little about a trapped crevice, and decide whether the first procurement action should be better drainage/cleanability, a different joint design, a verified alloy grade or a specialist assessment. This also prevents paying for a grade upgrade while leaving the actual salt-retention geometry unchanged.
7. Scope and unresolved evidence
- No matched 304/316/duplex test was found on the same caster geometry, fastener stack, bearing interface, surface finish and chloride exposure.
- ASSDA's ferric-chloride/washer temperatures and Outokumpu's ASTM G48 results are accelerated test data, not field-use temperature limits.
- BSSA's seawater guidance cannot be transferred numerically to every washdown or low-chloride environment.
- No exact stainless grade, material certificate, weld procedure, passivation record or chloride-corrosion test for this supplier's own caster products was available. No supplier-specific corrosion performance or guarantee is claimed.
- Actual local chloride concentration in evaporating films, deposit chemistry, crevice geometry and wet dwell for a buyer's installation remain to be measured or confirmed.
Conclusion: 316 is a meaningful improvement over 304 for some exposed-surface pitting conditions, but it is not a universal fix for chloride corrosion in wet caster joints. Qualify the assembly's drainage, crevice geometry, finish, deposits and actual exposure before approving a substitution.